Solvent popping
Source:The SiteAuthor:admin Addtime:2021/6/23 Click:0
Definition
-
Small bubbles in the top coat, some of them burst.
Cause
-
Excessive film thickness.
-
Top coat not allowed to flash off long enough before forced drying.
-
Specified spray viscosity not observed.
-
Unsuitable hardener or reducer.
Prevention
-
Apply paint in normal film thicknesses.
-
Keep to specified flash-off times.
-
Follow the instructions on spray viscosity, hardeners and reducers on the Technical Data Sheets.
Remedy
-
Sand the affected areas lightly with a sanding pad and respray within 24 hours. Do not sand pop marks open.
-
Where there are large bubbles / pop marks, sand down the surface completely and reapply the paint system.