Sanding marks
               Source:The SiteAuthor:admin Addtime:2021/6/23 Click:0
               
	
  
	
		
			
				Definition
			
			
				
					- 
						Sanding marks with swollen edges.
					
 
	 
 
	
		
			
				Cause
			
			
				
					- 
						Excessively coarse sanding materials for substrate preparation.
					
				Prevention
			
			
				
					- 
						Sand putty with P 120-180 (initial sanding) and P 240-320 (final sanding).
					
- 
						Surfacer: dry P 400-500, wet P 800-1200.
					
- 
						Follow instructions for substrate preparation on the Technical Data Sheets.
					
				Remedy
			
			
				
					- 
						When the top coat has fully dried, fine-sand and polish the paint surface.
					
- 
						To eliminate serious damage, sand paint surface and respray.